Variation in graphite removal from spent EV Black Mass
2024 (English)Independent thesis Advanced level (degree of Master (Two Years)), 20 credits / 30 HE credits
Student thesis
Abstract [en]
The Paris Agreement has accelerated the global transition to electric vehicles (EVs), with the market expected to grow to 300 million units by 2030. This surge will substantially increase the demand for raw materials, especially graphite, a critical component in lithium-ion batteries (LiBs), which require 50% more metals compared to conventional vehicles. Recycling spent batteries will be crucial to meeting this demand. By 2037, an estimated 7.25 million tons of black mass (BM) could be available for recycling, potentially yielding up to 2 million tons of graphite, further highlighting its significance in the clean energy transition.
This research focuses on investigating the variation in graphite recovery from BM using froth flotation, subsequent to thermal pre-treatment in two different types of equipment: a rotary kiln furnace (RK) and a microwave furnace (MW). The pre-treatment (BM-TT) was carried out in an inert nitrogen atmosphere under four different conditions: three distinct temperatures (200°C, 400°C, 600°C), and with the addition of calcium oxide (CaO) as a reaction medium at 400°C. Additionally, BM without any thermal treatment (BM-UT) was analyzed. Sieving analysis was performed to separate particles larger than 300 μm, which were further ground using a knife mill to enhance particle liberation. The -500 μm ground product was combined with the -300 μm sieved material, forming the flotation feed.
Froth flotation experiments were conducted using a 200 ml batch flotation cell (TU Clausthal design) under fixed conditions: 7 wt.% solids, an impeller speed of 85%, aeration at 4 L/min, and manual scraping every 5 seconds. Kerosene (350 g/ton) served as the collector, Methyl Isobutyl Carbinol (MIBC, 150 g/ton) as the frother, and water glass (1500 g/ton) as a dispersant in certain tests to mitigate particle aggregation. Reagent dosages were selected based on established literature.
The results reveal the impact of particle size after thermal treatment on flotation performance, particularly due to the generation of fine and ultrafine particles. A comparative analysis between the RK and MW treatments highlights differences in efficiency. Additionally, the influence of thermal treatment temperature on graphite recovery and separation efficiency was assessed, identifying the optimal conditions for maximum efficiency. Challenges such as poor separation efficiency, primarily due to the overflow (O/F) of lithium metal oxides (LMOs), were discussed, with recommendations for further studies to improve graphite selectivity in future recycling processes.
Furthermore, this study demonstrates the role of CaO as a reaction medium during thermal pre-treatment and its positive impact on selectivity in subsequent froth flotation analysis.
Place, publisher, year, edition, pages
2024.
Keywords [en]
black mass, froth flotation, thermal treatment, graphite, recovery
National Category
Geology
Identifiers
URN: urn:nbn:se:ltu:diva-109965OAI: oai:DiVA.org:ltu-109965DiVA, id: diva2:1897560
Subject / course
Student thesis, at least 30 credits
Educational program
Master Programme in Georesources Engineering
Supervisors
Examiners
2024-09-172024-09-132025-10-21Bibliographically approved